Default object view. Click to create a custom template, Node ID: 5361, Object ID: 5360

Trial #5

Trial #5

To evaluate compatibility of top cleaning alternatives with the tin metal strips used in the manufacture of solar cells.

2008

15

5

103

103

Part

04/02/2008

1,440.00

Immersion/Soak

Jason Marshall

Liquid
Tin

None

None

None

Gravimetric

Equal length strips of the supplied tin wire were cut to place in a 10 ml glass vial containing full strength products at room temperatures. Each strip was weighed to establish a baseline weight. Strips were immersed in a solution for 24 hours. The pieces were then removed and wiped to remove any residual cleaning product. Final weights were measured, and weight loss was determined. Observations were made during the 24-hour period.

During the compatibility test, no visual signs of damage were noted for any of the four products. Only one product, DS 144, had a weight change greater than 0.1%. One product, Ionox HC 2, had a slight increase in weight. Initial weights, final weights, weight change and percent change are listed in the table below.

Product Initial Wt Final Wt Change % Change
SC Actisolv 0.0981 0.0980 0.0001 0.10
Ionox HC 2 0.1058 0.1059 -0.0001 -0.09
DS 144 0.0970 0.0966 0.0004 0.41
IPA 0.0904 0.0903 0.0001 0.11

No significant change in weight was noted for any of the four products over a 24-hour period of immersion.

No relation

Name Class Section
Document Evaluation #0 Evaluation 3
Document Evaluation #1 Evaluation 3
Document Evaluation #2 Evaluation 3
Document Evaluation #3 Evaluation 3
Powered by eZ Publish™ CMS Open Source Web Content Management. Copyright © 1999-2014 eZ Systems AS (except where otherwise noted). All rights reserved.