Browse past lab clients by general industry sectors
Trial Purpose:
To remove silver polish from surface using immersion cleaning
Date Run:
12/16/2008Experiment Procedure:
Basic cleaning performance testing was conducted using ASTM G122 as the bases for cleaning.
Products were selected based on the compatibility of substrate and for removal of the contaminant. Five percent concentrations were used and heated the samples at 130F. The coupons were immersed in a product for 5 minutes, rinsed in tap water at 120 F and dried using compressed air at room temperature. Coupons were coated with silver polish using a handheld swab and allowed to dry for 120 minutes at room temperature. The contaminated coupons were weighed again to determine the amount of soil added. After cleaning process, the final weights were recorded, efficiencies were calculated and recorded.
Trial Results:
Cleaner | Initial wt | Final wt | % Removed |
Warren Chemical Company, Sea Wash 77 | |||
0.1794 | 0.0646 | 63.99 | |
0.5656 | 0.0870 | 84.62 | |
0.5122 | 0.1731 | 66.20 | |
A 1 Hydro Parke Hill, SW Wash 10 | |||
0.3957 | 0.0245 | 93.81 | |
0.4295 | 0.0714 | 83.38 | |
0.4371 | 0.0775 | 82.27 | |
Kyzen Company, Metalnox CP30 | |||
0.3151 | 0.0837 | 73.44 | |
0.4564 | 0.0590 | 87.07 | |
0.1348 | 0.0213 | 84.20 | |
Kyzen Company, Lonox 1 3302 | |||
0.7258 | 0.3062 | 57.81 | |
0.9183 | 0.0998 | 89.13 | |
-2.0812 | 0.0427 | 102.05 | |
Brulin Corporation, Nonsilicated H TP | |||
2.3856 | 0.0393 | 98.35 | |
1.4773 | 0.0232 | 98.43 | |
0.0939 | 0.0378 | 59.74 | |
Brulin Corporation, Safety Strip 58 | 98.00 | ||
0.2490 | 0.0050 | 97.99 | |
0.4646 | 0.1548 | 66.68 | |
0.0256 | 0.0052 | 79.69 |
Success Rating:
Preliminary compatibility tests on substrate coupons encouraging for at least one cleaning chemistry. More in-depth laboratory testing necessary.Conclusion:
Two products were effective in removing over 85% of the polish using immersion cleaning.